A study of natural pigment-based colour masterbatches has found that several commercial natural colorants can be compounded into poly(lactic acid) (PLA) and poly(butylene succinate) (PBS) on conventional twin-screw extrusion and injection molding equipment, with only limited changes to melt flow and mechanical performance. Heat sensitivity during processing and weak light fastness in service remain the constraints.
Four pigments, two biopolyesters
The researchers worked with four commercial natural pigments: blue spirulina, yellow curcumin, red beetroot and green chlorophyllin. Each was combined with PLA and with PBS to produce colour masterbatches by twin-screw extrusion. The formulations also contained titanium dioxide, calcium carbonate and stearic acid, added to support UV protection, dispersion and processing.
The masterbatches were then let down into the matching polymer matrix at 2, 4 and 6 wt% and molded into test specimens by injection molding, so that colour, flow behaviour and mechanical properties could be assessed at realistic addition levels.
The thermal window sets the limits
Natural pigments are organic structures that can begin to degrade at temperatures below those at which the carrier polymers are processed. Thermogravimetric analysis put degradation onset at approximately 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, while PLA and PBS degrade at considerably higher temperatures.
To keep exposure within bounds, the team selected extrusion profiles that melted each polymer while limiting the heat load on the pigment. Processing temperatures reached 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h.
Spirulina as the clear exception
That window suited most pigment–polymer combinations. Spirulina was the notable exception: during PLA processing it lost its characteristic blue colour, so a blue PLA masterbatch could not be produced. In PBS, whose lower processing temperature was gentler on the pigment, compounding succeeded. The result indicates that compatibility is governed less by the pigment alone than by the thermal processing requirements of the matrix it is dosed into.
Flow and mechanics stay close to baseline
From a processing standpoint the pigments caused only limited changes in rheology. Melt flow rate decreased slightly after incorporation, pointing to a modest increase in melt viscosity. Neat PLA measured about 50 g/10 min and the natural-pigment masterbatches stayed close to that figure; PBS showed a similar response, with only a minor reduction.
That matters for compounders, because a colour system offers little practical value if it forces major changes to screw design, pressure settings or molding conditions. In this work, conventional compounding and injection molding handled most formulations without major processing problems.
Tensile and impact behaviour were checked across the 2 to 6 wt% range. PLA started from a Young's modulus of about 1710 MPa and tensile strength of 65.6 MPa; PBS from about 392 MPa and 34.5 MPa. The coloured formulations stayed close to those baselines, and impact strength remained within a similar range, although individual pigments produced some variation.
Light fastness is the larger barrier
Successful extrusion did not ensure durable colour. After 50 hours of xenon-lamp exposure, most formulations showed a colour difference above ΔE* = 2, the level at which a change becomes visually perceptible. The main exception was the PLA formulation containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.
The study therefore points to UV stability as the largest barrier to broader use. Packaging, consumer products, agricultural parts and outdoor applications may require additional stabilization, protective coatings or pigment modification before natural colours can compete with conventional systems over long service periods.
An environmental advantage, under stated assumptions
On the environmental side the comparison favoured the natural route within the study's assumptions: one kilogram of curcumin pigment was associated with about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment. The natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.
The conclusion is that natural pigment masterbatches still need development, particularly in light fastness and thermal stability, but that several colorants can be compounded into PLA and PBS using conventional processing equipment with only limited changes in melt viscosity and mechanical performance. Further work, the researchers suggest, should focus on improving colour stability during processing and during subsequent service exposure.